True Fir (White Fir) Wood: Hardness and Weight

As an Amazon Affiliate we earn from qualifying purchases. All earnings are directly reinvested into this site to bring you free tutorials and project files - Thank you for your support!

White fir (Abies concolor) in numbers: hardness, weight, strength, shrinkage, movement and decay resistance, taken from the tables of the USDA Forest Products Laboratory’s Wood Handbook, followed by what the wood is like to work and what it is used for. The values are averages from small, clear, straight-grained test specimens; real boards with knots, sloping grain or a different moisture content will differ.

PropertyWhite fir
Janka side hardness, 12% moisture480 lbf (2,135 N)
Janka side hardness, green340 lbf
Hardness rankharder than 25 of the 168 woods with a 12% hardness value in our database
Density at 12% moisture27.3 lb/ft³ (437 kg/m³)
Weight per board foot (12%)2.27 lb
Specific gravity (ovendry weight, green volume)0.37
Specific gravity at 12% moisture0.39
Bending strength (modulus of rupture), 12%9,800 psi
Stiffness (modulus of elasticity), 12%1.5 million psi
Crushing strength (compression parallel to grain), 12%5,800 psi
Shrinkage green to ovendry: radial / tangential / volumetric3.3% / 7.0% / 9.8%
Tangential / radial shrinkage ratio2.12
Dimensional change per 1% moisture (radial / tangential)0.00112 / 0.00245
Impact bending (drop height to failure), 12%20 in.
Heartwood decay resistanceslightly or nonresistant

The species in this group

Lumber is often sold under a group name. These are the species the Wood Handbook reports for this group, with the same properties side by side.

SpeciesJanka (lbf)Density (lb/ft³)Bending (psi)Stiffness (Mpsi)Crushing (psi)Shrink T/R (%)Decay resistance
White fir
Abies concolor
48027.39,8001.55,8007.0 / 3.3slightly or nonresistant
Balsam fir
Abies balsamea
38024.59,2001.455,2806.9 / 2.9slightly or nonresistant
Grand fir
Abies grandis
49025.98,9001.575,2907.5 / 3.4slightly or nonresistant
Noble fir
Abies procera
41027.310,7001.726,1008.3 / 4.3slightly or nonresistant
California red fir
Abies magnifica
50026.610,5001.55,4607.9 / 4.5slightly or nonresistant
Pacific silver fir
Abies amabilis
43030.111,0001.766,4109.2 / 4.4slightly or nonresistant
Subalpine fir
Abies lasiocarpa
35022.48,6001.294,8607.4 / 2.6slightly or nonresistant
All values at 12% moisture content except shrinkage (green to ovendry). Where the Handbook gives one shrinkage value for a group, it is repeated for each species. Source: USDA Wood Handbook (FPL-GTR-190).

What it is

The true firs are the genus Abies. Six western species are cut for lumber: subalpine fir (A. lasiocarpa), California red fir (A. magnifica), grand fir (A. grandis), noble fir (A. procera), Pacific silver fir (A. amabilis) and white fir (A. concolor). They are cut mainly in Washington, Oregon, California, western Montana and northern Idaho and are marketed as white fir throughout the United States. The eastern species are balsam fir (A. balsamea), which grows mainly in New England, New York, Pennsylvania and the Great Lake States, and Fraser fir (A. fraseri) of the Appalachian Mountains of Virginia, North Carolina and Tennessee. Douglas-fir belongs to a different genus (Pseudotsuga).

The wood of the eastern true firs is creamy white to pale brown, with heartwood and sapwood generally indistinguishable, and the wood of the western firs is similar. The wood structure of the true firs is so alike that the species cannot be told apart by examining the wood alone.

Working properties

The western true firs are light in weight, and their shrinkage ranges from low to moderately high; white fir shrinks 7.0% tangentially from green to ovendry. Balsam and Fraser fir are lightweight, low in bending and compressive strength, moderately low in stiffness, soft and low in shock resistance. In the group table, subalpine fir is the lightest and softest of the seven.

Weight and density

At 12% moisture content white fir weighs about 27.3 lb per cubic foot, so one board foot (144 cubic inches) weighs about 2.27 lb. An 8 ft board of actual size 3/4 × 5-1/2 in. (a 1×6) holds 0.229 cubic feet and weighs about 6.3 lb; an 8 ft piece 1-1/2 × 3-1/2 in. (a 2×4 size) weighs about 8.0 lb. Green wood is much heavier because of the water it holds.

Density here is ovendry weight plus 12% water, divided by volume at 12% moisture content (Wood Handbook Eq. 4-12: density = specific gravity at 12% × 62.43 lb/ft³ × 1.12).

Wood movement

The Wood Handbook gives dimensional change coefficients for each species: the fraction of its width a board gains or loses for every 1% change in moisture content, between about 6% and 14%. For white fir they are 0.00245 across a flatsawn face (tangential) and 0.00112 across a quartersawn face (radial).

Worked example: a flatsawn board 7-1/4 in. wide (a nominal 1×8) that goes from 6% moisture content in a heated winter house to 12% in a humid summer changes width by 7.25 × 0.00245 × 6 = 0.107 in. (about 3/32 in.). The same board quartersawn moves 0.049 in. (about 1/16 in.). Allow for this in panels, tabletops and floors; the wood movement calculator works it out for any size and moisture range.

How it compares

SpeciesJanka (lbf)Density (lb/ft³)Bending (psi)Stiffness (Mpsi)Tangential shrink (%)Decay resistance
White fir48027.39,8001.57.0slightly or nonresistant
Douglas-fir (Coast)71033.612,4001.957.6moderately resistant
Western hemlock54031.511,3001.637.8slightly or nonresistant
Sitka spruce51028.010,2001.577.5slightly or nonresistant
Eastern white pine38024.58,6001.246.1moderately resistant (old growth only); otherwise slightly or nonresistant
Ponderosa pine46028.09,4001.296.2slightly or nonresistant
At 12% moisture content; shrinkage is green to ovendry. * density estimated from specific gravity; † density as stated in the Handbook text.

Uses

Western true fir lumber is used mainly for building construction, boxes and crates, planing-mill products, sashes, doors and general millwork. High-grade noble fir goes into interior woodwork, moulding, siding, sash and door stock, venetian blinds and ladder rails, and some of the highest quality material has been used in aircraft construction. The eastern firs are used mainly for pulpwood, with some lumber for structural products, especially in New England and the Great Lake States.

Frequently asked questions

How hard is white fir?

White fir averages 480 lbf (2,135 N) on the Janka test at 12% moisture content. The seven true firs in the Wood Handbook range from 350 lbf (subalpine fir) to 500 lbf (California red fir).

Is white fir the same as Douglas-fir?

No. Douglas-fir is a different genus and is harder and stronger: coast Douglas-fir averages 710 lbf and 12,400 psi in bending, against 480 lbf and 9,800 psi for white fir.

Can you tell the true firs apart?

Not from the wood. The Handbook says the wood structure of the true firs is so similar that the species cannot be distinguished by examining the wood alone, and the western species are marketed together as white fir.

Is fir good for outdoor use?

Not untreated. True fir heartwood is in the slightly or nonresistant decay class, which usually needs some form of preservative treatment where there is a decay hazard.

Sources

  1. USDA Forest Products Laboratory. Wood Handbook: Wood as an Engineering Material. General Technical Report FPL-GTR-190, 2010. Chapter 2 (species descriptions), Chapter 4 (Tables 4-3, 4-4 shrinkage; Eq. 4-7, 4-9, 4-12 density), Chapter 5 (Tables 5-3b, 5-5b strength and hardness), Chapter 13 (Table 13-5 dimensional change coefficients), Chapter 14 (Table 14-1 decay resistance)
  2. USDA Forest Products Laboratory. Wood Handbook, 2021 edition (FPL-GTR-282)

Last reviewed: 24 October 2026. Numbers are generated from our parsed copy of the Handbook tables, so every page uses the same data. Values marked * are estimates computed with the Handbook’s own equations. Spotted an error? Please let us know.